1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

HC#5 Clay

Description: Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.27% 0.02
K2O 0.31% 0.01
MgO 0.21% 0.02
Na2O 0.10% 0.01
TiO2 1.59% 0.07
Al2O3 27.65% 1.00
P2O5 0.14% -
SiO2 56.25% 3.45
Fe2O3 1.13% 0.03
MnO 0.02% -
LOI 12.40%n/a
SO3 0.03%n/a
Oxide Weight 323.41
Formula Weight 369.32

Notes

Particle Size Distribution:
>53 microns: 0.10 max
>10 microns: 18
<2 microns: 44

Modulus of Rupture, Kgf/cm2:
At 80% Relative Humidity: 7.5
Dried at 110C: 16.2

Casting Rate @ 62% solids (mm2/min): 2.0
% P84 Deflocculant Required for 5 Poise Slip: 0.6

1180C 1280C
Fired Absorption: 15% 6%
Fired Shrinkage: 9% 13%
Brightness: 84 84

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy