Bandy Tan

Alternate Names: Bandy Tan Ball Clay

Description: Ball clay

Oxide Analysis Formula Tolerance
CaO 0.32% 0.02
K2O 1.64% 0.07
MgO 0.58% 0.06
Na2O 0.36% 0.02
TiO2 1.26% 0.07
Al2O3 24.38% 1.00
P2O5 0.03% -
SiO2 61.21% 4.26
Fe2O3 1.20% 0.03
MnO 0.01% -
LOI 8.67%n/a
SO3 0.09%n/a
Oxide Weight 380.68
Formula Weight 417.23

Notes

Relative Viscosity (1.2 Sp. Gr.):* 1.2
Casting Rate: (gms per 15 min/426 cm2):* 157
Water of Plasticity:* 27.1
% Dry Shrinkage:* 5.1
Dry M.O.R., psi:* 228

Cone 04 8 11
----
Fired Shrinkage:* 0.4% 3.2% 6.4%
Absorption:* 21.3% 13.8% 5.9%
M.O.R. psi:* 745 2910 5680

Thermal Expansion, Cone 8: .335% at 700C
P.C.E.: 30
pH: 5.5
Oil Absorption: 34
Bulk Density, lbs per cubic foot: 37-45
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
95% 85% 66% 42% 26% 15% 3%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Frit Softening Point 30 PCE