Description: High alkali leadless aluminun silicate frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 13.96% | 0.41 | |
| K2O | 4.79% | 0.08 | |
| MgO | 0.86% | 0.03 | |
| Na2O | 18.10% | 0.48 | |
| TiO2 | 0.04% | - | |
| Al2O3 | 8.46% | 0.14 | |
| P2O5 | 0.03% | - | |
| SiO2 | 53.40% | 1.45 | |
| Fe2O3 | 0.37% | - | |
| Oxide Weight | 163.10 | ||
| Formula Weight | 163.10 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |