Alternate Names: CP #7 Ball Clay, CP#7 Clay, Spinks CP#7 Ball Clay
Description: Refractory ball clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.30% | 0.02 | |
| K2O | 0.26% | 0.01 | |
| MgO | 0.10% | 0.01 | |
| Na2O | 0.05% | - | |
| TiO2 | 1.60% | 0.07 | |
| Al2O3 | 28.70% | 1.00 | |
| P2O5 | 0.01% | - | |
| SiO2 | 54.90% | 3.25 | |
| Fe2O3 | 1.00% | 0.02 | |
| LOI | 12.50% | n/a | |
| SO3 | 0.20% | n/a | |
| Oxide Weight | 308.91 | ||
| Formula Weight | 353.85 | ||
The manufacturer describes it as a fine-grained engineered blend offering high Al2O3 percentage and excellent PCE characteristics. Excellent fired color an plasticity make this product ideally suited for refractory and dinnerware applications.
Relative Viscosity (1.2 Sp. Gr.):* 1.31
Casting Rate: (gms per 15 min/426 cm2):* 248
Water of Plasticity:* 20.2
% Dry Shrinkage:* 5.13
Dry M.O.R., psi:* 905
Cone 04 8 11
----
Fired Shrinkage:* 0.2% 1.9% 2.2%
Absorption:* 17.2% 13.4% 12.5%
M.O.R. psi:* 2320 4960 5790
Thermal Expansion, Cone 8: .535% at 700C
P.C.E.: 33
pH: 5.6
Oil Absorption: 35
Bulk Density, lbs per cubic foot: 33-38
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
96% 93% 83% 65% 46% 29% 12%
*Specimens: De-aired, extruded, 50% ball clay, 50% flint