| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.05% | - | |
| K2O | 2.20% | 0.07 | |
| MgO | 0.30% | 0.02 | |
| Na2O | 0.10% | - | |
| TiO2 | 0.05% | - | |
| Al2O3 | 36.50% | 1.00 | |
| SiO2 | 48.50% | 2.26 | |
| Fe2O3 | 0.85% | 0.01 | |
| LOI | 11.20% | n/a | |
| Oxide Weight | 247.45 | ||
| Formula Weight | 278.67 | ||
Particle Size Distribution:
>53 microns: 1.0 max
>10 microns: 18
<2 microns: 26
Modulus of Rupture, Kgf/cm2:
At 80% Relative Humidity: 3.0
Dried at 110C: 6.0
Casting Rate @ 65% solids (mm2/min): 6.5
% P84 Deflocculant Required for 5 Poise Slip: 0.40
1180C 1280C
Fired Absorption: 19% 11%
Fired Shrinkage: 6% 10%
Brightness: 84 86
| Materials |
Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries. |
| Typecodes |
Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content. |