Ultracast 760-C

Description: CLAY SLURRY

Oxide Analysis Formula Tolerance
CaO 0.10% 0.01
K2O 1.40% 0.06
MgO 0.30% 0.03
Na2O 0.16% 0.01
TiO2 1.61% 0.09
Al2O3 24.05% 1.00
SiO2 60.87% 4.30
Fe2O3 1.01% 0.03
LOI 10.28%n/a
Oxide Weight 379.58
Formula Weight 423.08

Notes

A clean kaolinitic ball clay slurry blend which exhibits superior properties for a variety of uses including fillter applications, ceramic tile body and glaze applications.

Specific Gravity: 1.605
% Solids: 61
Viscosity @ 90F (cps Brookfield, 100 rpm, spindle 3): 200-800
pH @90F: 5.7-6.3
CEC/MBI (meq/100 ml): 8.0-9.0
+200 mesh Residue (%): 0.0-1.0
+325 mesh Residue (%): 0.0-2.0
Soluble Sulfates (ppm): 150-350
Deflocculant Type: Sodium Silicate "N" Brand

Particle Size (% finer than):
5 microns: 86
1 micron: 63
0.5 microns: 53

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy