Ultracast 44 Slurry

Description: SANITARY WARE SLURRY

Oxide Analysis Formula Tolerance
CaO 0.10% 0.01
K2O 1.40% 0.06
MgO 0.30% 0.03
Na2O 0.16% 0.01
TiO2 1.61% 0.09
Al2O3 24.05% 1.00
SiO2 60.87% 4.30
Fe2O3 1.01% 0.03
LOI 10.28%n/a
Oxide Weight 379.58
Formula Weight 423.08

Notes

This slurry is intended to enhance casting qualities with faster casting rate as well as faster dewatering and set-up.

Crude Color: Dark Brown
% Solids: 60-61
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 520
Water of Plasticity (%): 33
Linear Dry Shrinkage (%): 5.6
Soluble Sulfates (ppm): 800-1200
Filtration (ml): 34
Specific Surface Area (sq meters per gram): 15.8
CEC/MBI (meq/100 ml): 7.0-7.5
pH @90F: 4.5-5.8
Specific Gravity: 1.59-1.61
Viscosity @ 90F (cps Brookfield, 100 rpm, spindle 3): 450-750
Casting Rate @ 90F, 15 min. (g): 45
Deflocculant Type: Sodium Silicate "N" Brand

Particle Size (% finer than):
5 microns: 77
1 micron: 44
0.5 microns: 33

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy