1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Sheffield Clay

Alternate Names: Shefield Clay

Description: Iron-rich native glacial clay

Oxide Analysis Formula Tolerance
CaO 3.20% 0.28
K2O 4.00% 0.21
MgO 3.50% 0.42
Na2O 1.20% 0.09
TiO2 1.00% 0.06
Al2O3 19.60% 0.93
SiO2 51.02% 4.13
Fe2O3 8.50% 0.26
LOI 8.00%n/a
Oxide Weight 447.33
Formula Weight 486.23

Notes

A native glacial iron-rich clay containing biotite, hornblende, chlorite, quartz, and other high Fe/Mg minerals. Sheffield Slip clay is based on this material.

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.
Materials Sheffield Slip

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy