S-3 Ball Clay

Alternate Names: s3 ball clay, Hick S-3, Old Hickory S-3 Ball Clay

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.02% -
K2O 1.10% 0.05
MgO 0.26% 0.03
Na2O 0.11% 0.01
TiO2 1.20% 0.06
Al2O3 24.00% 1.00
SiO2 61.20% 4.33
Fe2O3 1.04% 0.03
LOI 10.90%n/a
Oxide Weight 377.95
Formula Weight 424.19

Notes

Crude Color: Brown
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 407
Wet Sieve Residue, +200 mesh (%): 0.46
Water of Plasticity (%): 38
Linear Dry Shrinkage (%): 6.35
Solubles Sulfates (ppm): 560
Filtration (ml): 28
Specific Surface Area (sq meters per gram): 16.5
CEC/MBI (meq/100 ml): 8.5
pH: 4.7
PCE: 30

Firing Shrinkage (%) Cone 04: 4.5 Cone 3: 6.8 Cone 11: 8.9
Absorption (%) 21.6 12.7 5.6

Particle Size (% finer than):
50 microns: 100
20: 96
10: 94
5: 77
1: 48
0.5: 37

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.
By Tony Hansen