Description: Devon China Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.10% | - | |
| K2O | 2.40% | 0.07 | |
| MgO | 0.20% | 0.01 | |
| Na2O | 0.10% | - | |
| TiO2 | 0.40% | 0.01 | |
| Al2O3 | 36.50% | 1.00 | |
| SiO2 | 47.50% | 2.21 | |
| Fe2O3 | 1.00% | 0.02 | |
| LOI | 11.80% | n/a | |
| C | 0.10% | n/a | |
| Oxide Weight | 246.48 | ||
| Formula Weight | 279.77 | ||
Particle Size (e.s.d.)
125 microns - <0.1
10 microns - 87
2 microns - 42
1 microns - 28
Modulus of Rupture at 110C
Mn/M2 - 1.0
lbf/in2 - 140
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.2
Water Absorption
1120C - 20.5
1220C - 14.00
Shrinkage Dry to Fired
1120C - 10.00
1220C - 14.50
Reflectance 464nm
1120C - 84
1220C - 81
Refractoriness
Cone - 33, 1730C
| Materials |
Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries. |
| Typecodes |
Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content. |