Black Charm Clay

Alternate Names: Ball Charm Ball Clay

Description: Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.33% 0.03
K2O 1.34% 0.06
MgO 0.21% 0.02
Na2O 0.32% 0.02
TiO2 0.20% 0.01
Al2O3 22.66% 1.00
P2O5 0.04% -
SiO2 62.96% 4.72
Fe2O3 1.53% 0.04
MnO 0.05% -
LOI 10.52%n/a
SO3 0.11%n/a
Oxide Weight 403.50
Formula Weight 451.49

Notes

A coarse-grained engineered blend offering a high degree of moisture retention, plasticity, and naturally occurring organics. Ideally suited for a variety of bonding applications.

Relative Viscosity (1.2 Sp. Gr.):* 1.23
Casting Rate: (gms per 15 min/426 cm2):* 165
Water of Plasticity:* 26.4
% Dry Shrinkage:* 5.55
Dry M.O.R., psi:* 496

Cone 04 8 11
----
Fired Shrinkage:* 0.4% 1.5% 2.5%
Absorption:* 21.0% 18.3% 14.8%
M.O.R. psi:* 620 1830 4050

Thermal Expansion, Cone 8: .495% at 700C
P.C.E.: 29
pH: 4.6
Oil Absorption: 32
Bulk Density, lbs per cubic foot: 35-39
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
92% 81% 65% 45% 31% 16% 5%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Pyrometric Cone Equivalent 29
By Tony Hansen
Follow me on