1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

No. 6 DC

Alternate Names: Old Hickory No. 6 DC Ball Clay

Description: Kentucky Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.03% -
K2O 0.31% 0.01
MgO 0.20% 0.02
Na2O 0.10% 0.01
TiO2 1.80% 0.09
Al2O3 26.30% 1.00
SiO2 60.50% 3.90
Fe2O3 0.84% 0.02
LOI 9.70%n/a
Oxide Weight 349.36
Formula Weight 386.89

Notes

Crude Color: White
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 449
Wet Sieve Residue, +200 mesh (%): 0.31
Water of Plasticity (%): 33
Linear Dry Shrinkage (%): 5.02
Solubles Sulfates (ppm): 229
Filtration (ml): 26
Specific Surface Area (sq meters per gram): 17.3
CEC/MBI (meq/100 ml): 9.0
pH: 6.0
PCE: 32

Firing Shrinkage (%) Cone 04: 4.1 Cone 3: 6.6 Cone 11: 7.2
Absorption (%) 15.2 10.1 4.8

Particle Size (% finer than):
50 microns: 99
20: 97
10: 92
5: 85
1: 59
0.5: 48

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy