1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Minsilspar

Oxide Analysis Formula Tolerance
CaO 1.10% 0.15
K2O 2.80% 0.23
Na2O 4.90% 0.62
Al2O3 14.00% 1.07
SiO2 76.80% 9.96
Fe2O3 0.06% -
LOI 0.30%n/a
Oxide Weight 776.39
Formula Weight 778.72

Notes

Spruce Pine, NC
A 170 mesh feldspathic sand (sand-spar) product used primarily in the sanitary-ware industry.

Physical Properties
===================
Specific Gravity: 2.6
Refractive Index: 1.53
Mohs Hardness: 6-6.5
Mean Particle Size, microns: 19
Specific Surface Area, sq metre/g: 0.6-0.7
Dry Brightness (Green Filter): 91
Raw color:
pH: 8.2
% Moisture Content: 0.1
Bulk Density (lb/cu. ft)
Loose: 52
Packed: 83

Structure: Crystalline
Particle Shape: Granular

Particle Size: 100 140 170 200 325
% Retained 0.1 0.3 0.4 1.2 10.0
U.S. Sieve Series

Particle Size, Microns: 30 20 10 5
(% finer than) 75% 60% 30% 12%

Related Information

Links

Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy