Pemco Frit P-2V25

Alternate Names: 2V25,2V-25

Description: Low temperature flux frit used in brick coatings

Oxide Analysis Formula Tolerance
CaO 22.20% 0.55
MgO 3.00% 0.10
Na2O 15.30% 0.34
B2O3 21.50% 0.43
Al2O3 0.70% 0.01
SiO2 25.10% 0.58
F 12.20% 0.90
Oxide Weight 139.48
Formula Weight 139.48

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Hommel Frit 4GF45C
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 15.00
Co-efficient of Linear Expansion 15.0 x 10-6 (50-350C)
Frit Softening Point 1250F
Frit Melting Range (C) 1220-1270F
I.F.P. (celsius) 482C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy