1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Pemco Frit P-2D27

Alternate Names: 2D27,2D-27

Description: Leadless frit for use at cone 02-10

Oxide Analysis Formula Tolerance
CaO 6.60% 0.30
Na2O 16.80% 0.70
B2O3 19.50% 0.72
Al2O3 1.80% 0.05
SiO2 51.10% 2.19
F 4.20% 0.57
Oxide Weight 257.32
Formula Weight 257.32

Notes

Modification of P-835 adding fluorine. Used in same manner.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Pemco Frit P-835
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 11.70
Co-efficient of Linear Expansion 11.70 (50-450C)
Frit Softening Point 1300F
Frit Melting Range (C) 1280-1380F
Co-efficient of Linear Expansion 11.7x10-6 (50-450C)
I.F.P. (celsius) 528C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy