Ceradel Frit C 1250

Alternate Names: C1250 Fritte, C 1250 Fritte, Ceradel Frit 1250

Description: Lead bisilicate frit, Bisilicate de plomb

Oxide Analysis Formula Tolerance
SiO2 35.00% 2.00
PbO 65.00% 1.00
Oxide Weight 343.38
Formula Weight 343.38

Notes

The manufacturer calls this a lead bisilicate but only gives a range of values for the analysis (SiO2 - 15-40%, PbO 40-70%). Since the standard lead bisilicate is 65:35, that is what we have assigned here. We have another source that confirms that.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Lead Bisilicate Frit
A standard frit of 1 molar part of PbO and 2 of SiO2. It is considered stable and non-leachable.
Materials Ceradel Frit C 1249
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.

Data

Co-efficient of Linear Expansion 67 (10-7/C 20/300C)
Frit Softening Point 900-1100C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy