Potclays Frit 2279

Alternate Names: 2279 Fritte, Potclays Low Expansion Frit

Description: Alkali free calcium lithium magnesia zinc borosilicate frit

Oxide Analysis Formula Tolerance
CaO 3.60% 0.38
Li2O 0.10% 0.02
B2O3 17.80% 1.53
SiO2 63.60% 6.31
Al2O3 8.20% 0.48
ZnO 3.30% 0.24
MgO 2.40% 0.36
LOI 1.00%n/a
Oxide Weight 590.62
Formula Weight 596.58

Notes

We also have this slightly different analysis: CaO: 3.67, MgO: 2.05, ZnO: 2.85, B2O3: 17.92, Al2O3: 8.2, SiO2: 64.25, Li20: 1.06

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy