Frit A 2010

Description: Low melting lead borosilicate

Oxide Analysis Formula Tolerance
Na2O 6.00% 0.24
SiO2 13.00% 0.53
B2O3 12.00% 0.42
PbO 69.00% 0.76
Oxide Weight 246.36
Formula Weight 246.36

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Frit G-23
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 111 x 10-7 (20-400C)
Frit Softening Point 410C
Glass Transition Temperature 380C